Seven-Step Color Matching Method

2016-04-13

I. Clarify Color Matching Objectives

  1. Gain a clear and comprehensive understanding of the sample to be matched. Samples come in many forms: plastic parts, Pantone numbers, photographs, leather, metal components, or any other colored objects.
  2. Distinguish between soft and hard rubber colorants based on the plastic raw material, to narrow down the selection range of color powders.
  3. Select color powder or color masterbatch according to the molding process (e.g., medium-temperature resistant or high-temperature resistant color powder).
  4. Check for special requirements: weather resistance, chemical stability, addition of fillers or other additives, environmental compliance, etc.
  5. Confirm the required light source for color checking. Colors appear differently under natural light, fluorescent light, ultraviolet light and other light sources.

II. Analyze Hue

Principle for color matching: Adjust depth first, then hue, and fine-tune color difference at last. Depth can be adjusted using black/white color powders, as well as the concentration and saturation of colorants themselves.

Steps for hue analysis:

  1. Observe the transparency of the sample Samples are generally classified as transparent, translucent and opaque (also called solid color; high solid color means very low transparency). Two methods to adjust transparency: increase titanium dioxide content, or raise the saturation of color powder.
  2. Observe the sample surface ① If the sample surface has a whitish reflection (solid color with white undertone), titanium dioxide is present. Heavy whitish reflection indicates high titanium dioxide loading. ② Bright, high-chroma samples use less titanium dioxide and more chromatic color powder. (Higher colorant loading delivers brighter, deeper color; lower loading results in lighter, less luminous color.) ③ For deep, vivid samples with surface whitish reflection, increase both titanium dioxide and color powder dosage.

Note: Transparent samples require organic pigments or dyes with good transparency. For opaque or translucent samples, estimate titanium dioxide content by practical experience, then decide whether to add black pigment and its proportion based on hue.

III. Determine the Color Matching Formula

  1. First define titanium dioxide content — this is the core technical point. Any change in titanium dioxide will drastically alter the color and require adjustment of other color powder dosages.
  2. Analyze which pigments form the tone of the sample, identify the primary color and secondary colors, and estimate their proportions. (Select pigments with color undertones close to the sample. For red tones: use scarlet for yellowish samples; bright red or fluorescent red as primary color for vivid samples.)
  3. Check the chroma of the sample and evaluate whether fluorescent color powder or optical brightener is needed.

IV. Trial Compounding

  1. Select suitable color powders and build the preliminary formula based on the above analysis.
  2. Choose soft-rubber or hard-rubber grade, medium-temperature or high-temperature resistant color powder according to raw material type.
  3. Select pigments based on transparency, set titanium dioxide level and black/grey depth, then finalize color powder grades to match hue, depth and brightness.

V. Finalize the Formula

  1. Set titanium dioxide proportion
  2. Set black color powder proportion
  3. Set primary color powder proportion
  4. Set secondary color powder proportion (including dosage of fluorescent powder or optical brightener if required)

VI. Injection Molding Sampling / Fine Tuning

Note: Normally prepare 600 g of resin. Mix color powder and resin uniformly per formula, then produce test plaques via injection molding. After full cooling of test plaques, compare and analyze against the reference sample. Adjust color powder dosage according to hue, depth and chroma, repeat trials until the color meets requirements. (For computer color matching, perform data analysis based on deviations of L*, a*, b* values.)

VII. Notes for Matching Different Color Families

Example: White Series

  1. Finer titanium dioxide particles generally offer higher tinting strength. Dupont R105 is a common grade.
  2. White is widely used in light-colored plastic products, formulated with high titanium dioxide loading plus small amounts of pigments.
  3. For ultra-white shades, select titanium dioxide with a blue undertone.
  4. In PP/ABS systems, higher titanium dioxide content improves hiding power; hiding power plateaus above 8% loading.

Formula Example: PP Whitening White Formula (for door & window coating, MFI>35, as coating color masterbatch) (resin = 100 parts)